Purifying?agent?for?molten?zinc?in?HDG
Name:
Purifying?agent?for?molten?zinc?in?HDG
  • Model:
  • Uses:
  •  
Details

In the light of the high iron and impurity contents in molten zinc, poor fluidness and particles and fold on workpiece often occurred in hot galvanizing plants, our company has organized the famous specialists and scientific and technological personnel in many disciplines at home developed XY-XG-3 type purifying agent for molten zinc, a high and new technical product. It has effectively solved the difficult problem and filled in the gap in this field at home. Through testing and using, the agent reached the anticipated results and is well received by customers. At present the product is applying for a patent. 
Notice
Do well pretreatment work, do not carry the harmful impurity into zinc pot, galvanizing agent needs the acid and iron eliminating, and it would be best if rinsing water for pretreatment could be fluid.
Because of the high volatility of the agent, No.2 operation should be quickly performed.
In order to avoid the splashing of molten zinc causing danger, operators should be well dressed in labor protection articles. Operation with caution and safety first.
Purifying Treatment Method of Molten Zinc:
Keep furnace temperature at 450℃-470℃.
Place dry thermal insulation bricks (with strong water absorption) into box with holes, quickly pour the purifying agent to them, insert the box into molten zinc and move it back and forth until boiling ends, and take out the box with holes.
Eliminate suspended substances on the surface of molten zinc; scatter ammonium chloride (1-1.5 kg/ m2) to further eliminate impurity on the surface.
Repeat the abovementioned steps three or four times.
Add the alloy, which is 0.5% of molten zinc, in uniform distribution way. After all the melting, repeat the abovementioned step once. (If there are excessive aluminum or other alloys in original molten zinc, the step-by-step method can be used)
The temperature is controlled at 430℃-440℃ and the standing time is 6-12 h (time is as long as possible).
When small workpiece is tested (the temperature is at 430℃ and dipping time is not changed), the surface and coating thickness is measured. If the coating is thick, the alloy, which is 0.1 % of molten zinc, can be added. 
The zinc and the alloy can be added at one time until the alloy content in molten zinc reaches 1.5%.
After alloying is completed, the working temperature of molten zinc should be controlled at 440℃±5℃ and the lifting speed of traveling crane at 1.5 m / min.
 

 

返回頂部 電話
主站蜘蛛池模板: 国产剧情原创中文片在线 | 国产强奷免费在线 | 成人国产精品秘片多多 | 欧美日本一道免费一区三区 | 欧美老熟妇videos极品另类 | 丝袜美腿诱惑 | 精品无码自拍视频 | 国产熟妇与子伦hd | 无码专区无码专区视频网址 | 亚洲精品无码不卡av | 国产大屁股精品视频 | 亚洲综合久久成人A片红豆 亚洲综合久久精品无码色欲 | 亚洲国产欧美另类18不卡一区免费free | 欧美日韩精品视频一区在线观看 | 亚洲a∨天堂久久 | 日本一本二本无码免费视频 | 熟女人妇交换俱乐部 | 国产欧美日韩精品a在线观看 | 国产在线观看免费观看不卡 | 熟女毛毛多熟妇人妻AV | 亚洲欧美日本国产 | 亚洲国产精品嫩草影院永久 | 精品女同一区二区三区免费播 | 无码精品一区二区三区免费视频 | 久久久精品人妻无码专区不卡 | 欧美亚洲日韩国产网站 | 国产色精品久久人妻无码 | 亚洲精品欧美一区二区三区 | 日韩精品中文字幕视频一区 | 亚洲女同熟女一区二 | 人妻丰满熟妇av无码区免蜜臀 | 亚洲另类专区无码 | 精品在线观看一区 | 无码av在专区在线观看 | 曰本道久久综合久久爱 | 日本aⅴ大伊香蕉精品视频 人与性动交α欧美精品 | 亚洲av综合永久无码精品天堂 | 一级一毛片a级毛片 | 日韩美女爱爱视频一区 | 国产淫秽视频在线观看 | 免费日日夜夜影院的入口综合p |